Copper Alloys Search - Basic
Results
Copper Alloy C97300 Chemical Composition Element 53.0 8.0 1.5 17.0 11.0 58.0 11.0 3.0 25.0 1.5 0.05 14.0 0.005 0.50 0.08 0.35 0.15
Mechanical Properties* As Centrifugal Cast M02 30 Min for Standard 15 Min for Standard 8 Min for Standard As Continuous Cast M07 30 Min for Standard 15 Min for Standard 10 Min for Standard As Sand Cast As Sand Cast M01 30 Min for Standard 35 Typ 15 Min for Standard 17 Typ 8 Min for Standard 20 Typ 55 Typ
Physical Properties Melting Point - Liquidus°F 1904 Melting Point - Solidus°F 1850 Densitylb/cu in. at 68°F 0.321 Specific Gravity 8.89 Electrical Conductivity% IACS at 68°F 6 Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F 16.5 Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F) 9 Specific Heat CapacityBtu/ lb /°F at 68°F 0.09 Modulus of Elasticity in Tensionksi 16000
Fabrication Properties Soldering Excellent Brazing Excellent Oxyacetylene Welding Not Recommended Gas Shielded Arc Welding Not Recommended Coated Metal Arc Welding Not Recommended Machinability Rating 70
Thermal Properties Stress Relief 500 Solution Treatment 0
Typical uses Ornamental Castings Appearance Pleasing White Color Ornamental Castings Corrosion Resistance Corrosion Resistance (Excellent) Ornamental Castings Machining Properties Machinability, Good Ornamental Castings Mechanical Properties Moderate Strength Statuary Appearance Pleasing White Color Statuary Corrosion Resistance Corrosion Resistance (Excellent) Statuary Machining Properties Machinability, Good Statuary Mechanical Properties Moderate Strength Hardware Appearance Pleasing White Color Hardware Corrosion Resistance Corrosion Resistance (Excellent) Hardware Machining Properties Machinability, Good Hardware Mechanical Properties Moderate Strength Valves Corrosion Resistance Corrosion Resistance (Excellent) Valves Machining Properties Machinability, Good Valves Mechanical Properties Moderate Strength
Applicable Specifications Standard Description As Centrifugal Cast Castings ASTM B271/B271M COPPER BASE ALLOY CENTRIFUGAL CASTINGS As Continuous Cast Castings ASTM B505/B505M COPPER BASE ALLOY CONTINUOUS CASTINGS Castings SAE J461 WROUGHT AND CAST COPPER ALLOYS Castings SAE J462 CAST COPPER ALLOYS As Sand Cast Castings ASTM B584 COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS Castings ASTM B763/B763M COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS Ingot ASTM B30 COPPER BASE ALLOYS IN INGOT FORM
No information available.
PLEASE NOTE: This search is best used with Chrome, FFox 3.6+, Safari 2+, Opera 10+ and IE 9+. To report an issue with this page, please
contact us .
DISCLAIMER: The values listed above represent reasonable approximations suitable for general engineering use. Due to commercial variations in compositions and to manufacturing limitations, they should not be used for specification purposes. See applicable ASTM International specification references.