Loading...
Copper Alloys Search - Basic
Results
C95800
Cast
BRONZES
Copper-Aluminum-Iron and Copper-Aluminum-Iron-Nickel Alloys (Aluminium Bronzes)
true
true
https://api.copper.org/alloys.xhtml/C95800
Elements | |||||||
---|---|---|---|---|---|---|---|
Cu(1) | Pb | Fe(2) | Ni(3) | Al | Mn | Si | |
(1) Cu + Sum of Named Elements 99.5% min. (2) Fe content shall not exceed Ni content. (3) Fe content shall not exceed Ni content. |
|||||||
Min (%) | 79.0 | 3.5 | 4.0 | 8.5 | 0.8 | ||
Max (%) | 0.03 | 4.5 | 5.0 | 9.5 | 1.5 | 0.10 |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Brinell Hardness, 3000 kg load | Shear Strength (ksi) |
Izod (ft-lbs) |
Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .001 in. set/in. (ksi) |
Compressive Strength .01 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
Fatigue Strength** (ksi) |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||||
As Centrifugal Cast | As Centrifugal Cast | M02 |
85 Min for Standard 85 Min for Standard |
35 Min for Standard |
15 Min for Standard 15 Min for Standard |
|||||||||
As Continuous Cast | As Continuous Cast | M07 |
85 Min for Standard 85 Min for Standard |
35 Min for Standard |
18 Min for Standard 18 Min for Standard |
|||||||||
As Permanent Mold Cast | As Permanent Mold Cast | M05 |
90 Min for Standard 96 Typ |
40 Min for Standard 52 Typ |
15 Min for Standard 17 Typ |
88 Typ |
||||||||
As Sand Cast | As Sand Cast | M01 |
85 Min for Standard 85 Min for Standard 95 Typ |
35 Min for Standard 38 Typ |
15 Min for Standard 15 Min for Standard 25 Typ |
159 Typ |
58 Typ |
20 Typ | 16 Typ |
35 Typ | 48 Typ | 100 Typ | 31 Typ |
(1)Field Sterength 16 kA/m | |
Melting Point - Liquidus°F | 1940 |
---|---|
Melting Point - Solidus°F | 1910 |
Densitylb/cu in. at 68°F | 0.276 |
Specific Gravity | 7.64 |
Electrical Conductivity% IACS at 68°F | 7 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 20.8 |
Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.105 |
Modulus of Elasticity in Tensionksi | 16500 |
Magnetic Permeability | 1.05 (1) |
Poisson's Ratio | 0.32 |
Casting Attribute | Level |
---|---|
Casting Yield | Low |
Drossing | High |
Effect of Section Size | Low |
Fluidity | Medium |
Gassing | Medium |
Patternmakers Shrinkage inches per inch | 3/16 |
Shrinkage in Solidification | High |
Technique | Suitability |
---|---|
Soldering | Good |
Brazing | Fair |
Oxyacetylene Welding | Not Recommended |
Gas Shielded Arc Welding | Good |
Coated Metal Arc Welding | Good |
Machinability Rating | 20 |
Common Fabrication Processes
No fabrication process properties for this alloy
Treatment | Value* | Time** | ||
---|---|---|---|---|
* Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
Stress Relief | 600 | |||
Solution Treatment | 0 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Fasteners | Nuts | Corrosion Resistance | Corrosion Resistance (Excellent) |
Nuts | Machining Properties | Machinability, Good | |
Nuts | Mechanical Properties | High Strength | |
Industrial | Bushings | Corrosion Resistance | Corrosion Resistance (Excellent) |
Bushings | Friction & Wear Properties | Wear Resistance | |
Bushings | Machining Properties | Machinability, Good | |
Bushings | Mechanical Properties | High Strength | |
Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Gears | Friction & Wear Properties | Wear Resistance | |
Gears | Machining Properties | Machinability, Good | |
Gears | Mechanical Properties | High Strength | |
Machinery | Conductivity (Thermal) | Thermal Conductivity | |
Machinery | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Machinery | Friction & Wear Properties | Wear Resistance | |
Machinery | Mechanical Properties | High Strength | |
Pickling Equipment | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pickling Equipment | Corrosion Resistance | Corrosion Resistance to Acids | |
Pickling Equipment | Mechanical Properties | High Strength | |
Propeller Blades | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Propeller Blades | Friction & Wear Properties | Wear Resistance | |
Propeller Blades | Mechanical Properties | Fatigue Strength | |
Propeller Blades | Mechanical Properties | High Strength | |
Propeller Hub | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Propeller Hub | Friction & Wear Properties | Wear Resistance | |
Propeller Hub | Mechanical Properties | Fatigue Strength | |
Propeller Hub | Mechanical Properties | High Strength | |
Shafts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Shafts | Friction & Wear Properties | Wear Resistance | |
Shafts | Mechanical Properties | High Strength | |
Valve Bodies | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valve Bodies | Friction & Wear Properties | Wear Resistance | |
Valve Bodies | Mechanical Properties | High Strength | |
Wear Plates | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Wear Plates | Friction & Wear Properties | Wear Resistance | |
Wear Plates | Mechanical Properties | High Strength | |
Worm Wheels | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Worm Wheels | Friction & Wear Properties | Wear Resistance | |
Worm Wheels | Machining Properties | Machinability, Good | |
Worm Wheels | Mechanical Properties | High Strength | |
Worms | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Worms | Friction & Wear Properties | Wear Resistance | |
Worms | Mechanical Properties | High Strength | |
Marine | Covers for Marine Hardware | Appearance | Appearance |
Covers for Marine Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Covers for Marine Hardware | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
Covers for Marine Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Covers for Marine Hardware | Mechanical Properties | High Strength | |
Marine Hardware | Appearance | Appearance | |
Marine Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Marine Hardware | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Marine Hardware | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
Marine Hardware | Mechanical Properties | High Strength | |
Ship Building | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Ship Building | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
Ship Building | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Ship Building | Friction & Wear Properties | Wear Resistance | |
Ship Building | Mechanical Properties | High Strength | |
Valves in contact with sea water. | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valves in contact with sea water. | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Valves in contact with sea water. | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
Valves in contact with sea water. | Friction & Wear Properties | Wear Resistance | |
Valves in contact with sea water. | Mechanical Properties | High Strength | |
Plumbing | Elbows | Corrosion Resistance | Corrosion Resistance (Excellent) |
Elbows | Machining Properties | Machinability, Good | |
Elbows | Mechanical Properties | High Strength | |
Elbows | Mechanical Properties | Retains Strength at Elevated Temperatures |
Form | Specific Sub-Form | Application | System | Standard | Description |
---|---|---|---|---|---|
As Centrifugal Cast | Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | ||
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
As Continuous Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | ||
Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
As Sand Cast | Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | ||
Castings | ASTM | B148 | ALUMINUM BRONZE SAND CASTINGS | ||
Castings | MILITARY | MIL-B-24480 | BRONZE, NICKEL-ALUMINUM CASTINGS, FOR SEAWATER SERVICE | ||
Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | ||
Ingot | |||||
ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | |||
Precision Cast | Castings | ASTM | B806 | PERMANENT MOLD CASTINGS | |
Valves |
Corrosion Properties
No Corrosion Properties Available.
DOWNLOAD Standard Designation for Wrought and Cast Alloys [PDF 775KB, includes all alloys]
PLEASE NOTE: This search is best used with Chrome, FFox 3.6+, Safari 2+, Opera 10+ and IE 9+. To report an issue with this page, please contact us.
DISCLAIMER:
The values listed above represent reasonable approximations suitable for general engineering use. Due to commercial variations in compositions and to manufacturing limitations, they should not be used for specification purposes. See applicable ASTM International specification references.