Loading...
Copper Alloys Search - Basic
Results
C95400CastBRONZESCopper-Aluminum-Iron and Copper-Aluminum-Iron-Nickel Alloys (Aluminium Bronzes)TrueTruehttps://api.copper.org/CDA-API/alloys.xhtml/C95400
Element | |||||
---|---|---|---|---|---|
Cu(1) | Fe | Ni(2) | Al | Mn | |
(1) Cu + Sum of Named Elements 99.5% min. (2) Ni value includes Co. | |||||
Min (%) | 83.0 | 3.0 | 10.0 | ||
Max (%) | 5.0 | 1.5 | 11.5 | 0.50 |
Form | Temper | Temper Code | Tensile Strength (ksi) | YS-0.5% Ext (ksi) | Elongation (%) | Brinell Hardness, 3000 kg load | Shear Strength (ksi) | Izod (ft-lbs) | Charpy V-Notch Impact Strength (ft-lbs) | Charpy Un-Notched Impact Strength | Compressive Strength .1 in. set/in. (ksi) | Creep Strength (0.1% per 10,000 hours) (ksi) | Fatigue Strength** (ksi) | Proportional Limit (ksi) | ||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
As Centrifugal Cast | As Centrifugal Cast | M02 | 75 Min for Standard 75 Min for Standard 75 Min for Standard | 30 Min for Standard 30 Min for Standard 30 Min for Standard | 12 Min for Standard 12 Min for Standard | 150 Min for Standard | ||||||||||
Quenched Hardened and Temper Annealed | TQ50 | 90 Min for Standard 90 Min for Standard | 45 Min for Standard 45 Min for Standard | 6 Min for Standard 6 Min for Standard | 190 Min for Standard | |||||||||||
As Continuous Cast | As Continuous Cast | M07 | 85 Min for Standard 85 Min for Standard | 32 Min for Standard 32 Min for Standard | 12 Min for Standard 12 Min for Standard | |||||||||||
Quenched Hardened and Temper Annealed | TQ50 | 95 Min for Standard 95 Min for Standard | 45 Min for Standard 45 Min for Standard | 10 Min for Standard 10 Min for Standard | ||||||||||||
As Permanent Mold Cast | As Permanent Mold Cast | M05 | 100 Min for Standard 105 Typ | 40 Min for Standard 46 Typ | 10 Min for Standard 11 Typ | |||||||||||
As Sand Cast | As Sand Cast | M01 | 75 Min for Standard 75 Min for Standard | 30 Min for Standard 30 Min for Standard | 12 Min for Standard | 150 Min for Standard | ||||||||||
M01 | 75 Min for Standard 75 Min for Standard 75 Min for Standard 85 Typ | 30 Min for Standard 30 Min for Standard 30 Min for Standard 35 Typ | 12 Min for Standard 12 Min for Standard 18 Typ | 150 Min for Standard 170 Typ | 47 Typ | 16 Typ | 11 Typ | 100 Typ | 7.4 Typ 2.9 Typ 17 Typ 4.4 Typ | 28 Typ | 17 Typ | |||||
Quenched Hardened and Temper Annealed | TQ50 | 90 Min | 45 Min | 6 Min | 190 Min | |||||||||||
TQ50 | 90 Min for Standard 90 Min for Standard 105 Typ | 45 Min for Standard 45 Min for Standard 54 Typ | 6 Min for Standard 6 Min for Standard 8 Typ | 190 Min for Standard 195 Typ | 50 Typ | 11 Typ | 7 Typ | 120 Typ | 35 Typ | 28 Typ | ||||||
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. |
(1) As Cast, Field Strength 16 kA/m | |
(2) TQ 50 Temper, Field Sterngth 16 kA/m | |
Melting Point - Liquidus°F | 1900 |
---|---|
Melting Point - Solidus°F | 1880 |
Densitylb/cu in. at 68°F | 0.269 |
Specific Gravity | 7.45 |
Electrical Conductivity% IACS at 68°F | 13 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 33.9 |
Coefficient of Thermal Expansion 68-57210⁻⁶ per °F (68 – 572°F) | 9 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.1 |
Modulus of Elasticity in Tensionksi | 15500 |
Magnetic Permeability | 1.27(1) |
Magnetic Permeability | 1.2(2) |
Technique | Suitability |
---|---|
Soldering | Good |
Brazing | Good |
Oxyacetylene Welding | Not Recommended |
Gas Shielded Arc Welding | Good |
Coated Metal Arc Welding | Good |
Machinability Rating | 60 |
Common Fabrication Processes
- Casting
Treatment | Minimum* | Maximum* | Value* | Time** | Medium |
---|---|---|---|---|---|
* Temperature is measured in Fahrenheit. ** Time is measured in minutes. | |||||
Stress Relief | 600 | ||||
Solution Treatment | 1600 | 1675 | 1 | Water | |
Annealing | 1150 | 1225 | 1 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Automotive | Weld Guns | Conductivity (Thermal) | Thermal Conductivity |
Weld Guns | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Weld Guns | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Weld Guns | Friction & Wear Properties | Wear Resistance | |
Weld Guns | Machining Properties | Machinability, Good | |
Weld Guns | Mechanical Properties | High Strength | |
Weld Guns | Mechanical Properties | Moderate Strength | |
Weld Guns | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Fasteners | Large Hold Down Screws | Corrosion Resistance | Corrosion Resistance (Excellent) |
Large Hold Down Screws | Machining Properties | Machinability, Good | |
Large Hold Down Screws | Mechanical Properties | High Strength | |
Nuts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Nuts | Mechanical Properties | High Strength | |
Industrial | Bearing Segments for the Steel Industry | Corrosion Resistance | Corrosion Resistance (Excellent) |
Bearing Segments for the Steel Industry | Friction & Wear Properties | Wear Resistance | |
Bearing Segments for the Steel Industry | Mechanical Properties | High Strength | |
Bearing Segments for the Steel Industry | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Bearing Segments for the Steel Industry | Mechanical Properties | Toughness | |
Bearings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Bearings | Friction & Wear Properties | Wear Resistance | |
Bearings | Mechanical Properties | High Strength | |
Bearings | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Bearings | Mechanical Properties | Toughness | |
Bushings | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Bushings | Friction & Wear Properties | Wear Resistance | |
Bushings | Machining Properties | Machinability, Good | |
Bushings | Mechanical Properties | High Strength | |
Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Gears | Friction & Wear Properties | Wear Resistance | |
Gears | Machining Characteristics | Excellent Machinability | |
Gears | Mechanical Properties | High Strength | |
Heavily Loaded Worm Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Heavily Loaded Worm Gears | Friction & Wear Properties | Wear Resistance | |
Heavily Loaded Worm Gears | Machining Properties | Machinability, Good | |
Heavily Loaded Worm Gears | Mechanical Properties | High Strength | |
High Strength Clamps | Corrosion Resistance | Corrosion Resistance (Excellent) | |
High Strength Clamps | Mechanical Properties | High Strength | |
Landing Gear Parts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Landing Gear Parts | Friction & Wear Properties | Wear Resistance | |
Landing Gear Parts | Mechanical Properties | Fatigue Properties | |
Landing Gear Parts | Mechanical Properties | High Strength | |
Machine Parts | Conductivity (Thermal) | Thermal Conductivity | |
Machine Parts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Machine Parts | Friction & Wear Properties | Wear Resistance | |
Machine Parts | Machining Characteristics | Excellent Machinability | |
Machine Parts | Mechanical Properties | High Strength | |
Machine Parts | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Pawl | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pawl | Friction & Wear Properties | Wear Resistance | |
Pawl | Mechanical Properties | High Strength | |
Pickling Hooks | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pickling Hooks | Corrosion Resistance | Corrosion Resistance to Acids | |
Pickling Hooks | Friction & Wear Properties | Wear Resistance | |
Pickling Hooks | Mechanical Properties | High Strength | |
Pressure Blocks for the Steel Industry | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pressure Blocks for the Steel Industry | Friction & Wear Properties | Wear Resistance | |
Pressure Blocks for the Steel Industry | Mechanical Properties | High Strength | |
Pressure Blocks for the Steel Industry | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Pump Parts | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pump Parts | Friction & Wear Properties | Wear Resistance | |
Pump Parts | Machining Properties | Machinability, Good | |
Pump Parts | Mechanical Properties | High Strength | |
Spur Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Spur Gears | Friction & Wear Properties | Wear Resistance | |
Spur Gears | Mechanical Properties | High Strength | |
Valve Bodies | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valve Bodies | Friction & Wear Properties | Wear Resistance | |
Valve Bodies | Machining Properties | Machinability, Good | |
Valve Bodies | Mechanical Properties | High Strength | |
Valve Guides | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valve Guides | Friction & Wear Properties | Wear Resistance | |
Valve Guides | Mechanical Properties | High Strength | |
Valve Seats | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valve Seats | Friction & Wear Properties | Wear Resistance | |
Valve Seats | Machining Characteristics | Excellent Machinability | |
Valve Seats | Mechanical Properties | High Strength | |
Valves | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Valves | Friction & Wear Properties | Wear Resistance | |
Valves | Machining Properties | Machinability, Good | |
Valves | Mechanical Properties | High Strength | |
Worm Gears | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Worm Gears | Friction & Wear Properties | Wear Resistance | |
Worm Gears | Machining Properties | Machinability, Good | |
Worm Gears | Mechanical Properties | High Strength | |
Marine | Covers for Marine Hardware | Appearance | Appearance |
Covers for Marine Hardware | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Covers for Marine Hardware | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Covers for Marine Hardware | Mechanical Properties | High Strength | |
Ship Building | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Ship Building | Corrosion Resistance | Corrosion Resistance to Salt Water | |
Ship Building | Friction & Wear Properties | Wear Resistance | |
Ship Building | Mechanical Properties | High Strength | |
Ordnance | Government Fittings | Corrosion Resistance | Corrosion Resistance (Excellent) |
Government Fittings | Friction & Wear Properties | Wear Resistance | |
Government Fittings | Machining Characteristics | Excellent Machinability | |
Government Fittings | Mechanical Properties | High Strength |
Form | Sub-Form | System | Standard | Description |
---|---|---|---|---|
As Centrifugal Cast | Castings | ASME | SB271 | COPPER BASE ALLOY CENTRIFUGAL CASTINGS |
Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | |
As Continuous Cast | Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | |
As Permanent Mold Cast | Castings | ASTM | B806 | PERMANENT MOLD CASTINGS |
As Sand Cast | Castings | ASME | SB148 | ALUMINUM BRONZE SAND CASTINGS |
Castings | ASTM | B148 | ALUMINUM BRONZE SAND CASTINGS | |
ASTM | B66 | BRONZE CASTINGS IN THE ROUGH FOR LOCOMOTIVE WEARING PARTS | ||
Castings | ASTM | B763/B763M | COPPER ALLOY SAND CASTINGS FOR VALVE APPLICATIONS | |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |
Castings | SAE | J462 | CAST COPPER ALLOYS | |
Ingot | ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | |
Precision Cast | Castings | MILITARY | MIL-C-11866 | CASTINGS, PRECISION, NONFERROUS |
Corrosion Properties
No information available.
DOWNLOAD Standard Designation for Wrought and Cast Alloys [PDF 775KB, includes all alloys]
PLEASE NOTE: This search is best used with Chrome, FFox 3.6+, Safari 2+, Opera 10+ and IE 9+. To report an issue with this page, please contact us.
DISCLAIMER:
The values listed above represent reasonable approximations suitable for general engineering use. Due to commercial variations in compositions and to manufacturing limitations, they should not be used for specification purposes. See applicable ASTM International specification references.