Elements | |||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|
Cu(1,2) | Pb | Sn | Zn | Fe | P(3) | Ni(4) | Al | S | Sb | Si | |
(1) In determining Cu min., Cu may be calculated as Cu + Ni. (2) Cu + Sum of Named Elements 99.3% min. (3) For continuous castings P shall be 1.5% max. (4) Ni value includes Co. |
|||||||||||
Min (%) | 86.0 | 1.0 | 5.5 | 3.0 | |||||||
Max (%) | 90.0 | 2.0 | 6.5 | 5.0 | 0.25 | 0.05 | 1.0 | 0.005 | 0.05 | 0.25 | 0.005 |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Brinell Hardness, 500 kg load | Charpy V-Notch Impact Strength (ft-lbs) |
Compressive Strength .001 in. set/in. (ksi) |
Compressive Strength .01 in. set/in. (ksi) |
Compressive Strength .1 in. set/in. (ksi) |
Creep Strength (0.1% per 10,000 hours) (ksi) |
Fatigue Strength** (ksi) |
---|---|---|---|---|---|---|---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | ||||||||||||
As Centrifugal Cast | As Centrifugal Cast | M02 |
34 Min for Standard 34 Min for Standard |
16 Min for Standard |
22 Min for Standard 22 Min for Standard |
|||||||
As Continuous Cast | As Continuous Cast | M07 |
38 Min for Standard 38 Min for Standard |
19 Min for Standard |
18 Min for Standard 18 Min for Standard |
|||||||
As Permanent Mold Cast | As Permanent Mold Cast | M05 |
34 Min for Standard |
16 Min for Standard |
24 Min for Standard |
|||||||
As Sand Cast | As Sand Cast | M01 |
34 Min for Standard 34 Min for Standard 40 Typ |
16 Min for Standard 20 Typ |
22 Min for Standard 22 Min for Standard 30 Typ |
65 Typ |
19 Typ |
15 Typ | 20 Typ | 38 Typ | 11 Typ | 11 Typ |
Melting Point - Liquidus°F | 1810 |
---|---|
Melting Point - Solidus°F | 1518 |
Densitylb/cu in. at 68°F | 0.312 |
Specific Gravity | 8.64 |
Electrical Conductivity% IACS at 68°F | 14 |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 40.2 |
Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 10 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.09 |
Modulus of Elasticity in Tensionksi | 14000 |
Incipient Melting°F | 600 |
Magnetic Permeability | 1 |
Casting Attribute | Level |
---|---|
Casting Yield | Medium |
Drossing | Low |
Effect of Section Size | High |
Fluidity | Medium |
Gassing | Medium |
Patternmakers Shrinkage inches per inch | 3/16 |
Shrinkage in Solidification | Low |
Technique | Suitability |
---|---|
Soldering | Excellent |
Brazing | Excellent |
Oxyacetylene Welding | Not Recommended |
Gas Shielded Arc Welding | Not Recommended |
Coated Metal Arc Welding | Not Recommended |
Machinability Rating | 42 |
Common Fabrication Processes
No fabrication process properties for this alloy
Treatment | Value* | Time** | ||
---|---|---|---|---|
* Temperature is measured in Fahrenheit. ** Time is measured in minutes. | ||||
Stress Relief | 500 | |||
Solution Treatment | 0 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Architecture | Ornamental Castings | Corrosion Resistance | Corrosion Resistance |
Ornamental Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Ornamental Castings | Machining Properties | Machinability, Good | |
Ornamental Castings | Mechanical Properties | Moderate Strength | |
Building | Cooling Equipment | Conductivity (Thermal) | Thermal Conductivity |
Cooling Equipment | Corrosion Resistance | Corrosion Resistance | |
Cooling Equipment | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Cooling Equipment | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
Cooling Equipment | Machining Properties | Machinability, Good | |
Cooling Equipment | Mechanical Properties | Moderate Strength | |
Cooling Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Cooling Equipment | Pressure Tight | Pressure Tight up to 260 C | |
Heating Equipment | Conductivity (Thermal) | Thermal Conductivity | |
Heating Equipment | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Heating Equipment | Machining Properties | Machinability, Good | |
Heating Equipment | Mechanical Properties | Moderate Strength | |
Heating Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Heating Equipment | Pressure Tight | Pressure Tight up to 260 C | |
Fasteners | Nuts | Corrosion Resistance | Corrosion Resistance |
Nuts | Machining Properties | Machinability, Good | |
Nuts | Mechanical Properties | Moderate Strength | |
Industrial | Bearings | Corrosion Resistance | Corrosion Resistance |
Bearings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Bearings | Friction & Wear Properties | Wear Resistance | |
Bearings | Machining Properties | Machinability, Good | |
Bearings | Mechanical Properties | Moderate Strength | |
Bushings | Corrosion Resistance | Corrosion Resistance | |
Bushings | Friction & Wear Properties | Wear Resistance | |
Bushings | Machining Properties | Machinability, Good | |
Bushings | Mechanical Properties | Moderate Strength | |
Cryogenic Valves | Corrosion Resistance | Corrosion Resistance | |
Cryogenic Valves | Machining Properties | Machinability, Good | |
Cryogenic Valves | Mechanical Properties | Moderate Strength | |
Cryogenic Valves | Pressure Tight | Pressure Tight up to 260 C | |
Fittings Used to 550 F | Corrosion Resistance | Corrosion Resistance | |
Fittings Used to 550 F | Machining Properties | Machinability, Good | |
Fittings Used to 550 F | Mechanical Properties | Moderate Strength | |
Fittings Used to 550 F | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Gears | Corrosion Resistance | Corrosion Resistance | |
Gears | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Gears | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
Gears | Friction & Wear Properties | Wear Resistance | |
Gears | Machining Properties | Machinability, Good | |
Gears | Mechanical Properties | Moderate Strength | |
Medium Pressure Hydraulic Equipment | Corrosion Resistance | Corrosion Resistance | |
Medium Pressure Hydraulic Equipment | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Medium Pressure Hydraulic Equipment | Machining Properties | Machinability, Good | |
Medium Pressure Hydraulic Equipment | Mechanical Properties | Moderate Strength | |
Medium Pressure Hydraulic Equipment | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Medium Pressure Hydraulic Equipment | Pressure Tight | Pressure Tight up to 260 C | |
Piston Rings | Corrosion Resistance | Corrosion Resistance | |
Piston Rings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Piston Rings | Machining Properties | Machinability, Good | |
Piston Rings | Mechanical Properties | Moderate Strength | |
Piston Rings | Pressure Tight | Pressure Tight up to 260 C | |
Pump Impellers | Corrosion Resistance | Corrosion Resistance (Excellent) | |
Pump Impellers | Machining Properties | Machinability, Good | |
Pump Impellers | Mechanical Properties | Moderate Strength | |
Pumps Used to 550 F | Corrosion Resistance | Corrosion Resistance | |
Pumps Used to 550 F | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Pumps Used to 550 F | Corrosion Resistance | Resistant in Saline Solutions | |
Pumps Used to 550 F | Friction & Wear Properties | Wear Resistance | |
Pumps Used to 550 F | Machining Properties | Machinability, Good | |
Pumps Used to 550 F | Mechanical Properties | Moderate Strength | |
Pumps Used to 550 F | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Valve Components | Corrosion Resistance | Corrosion Resistance | |
Valve Components | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Valve Components | Corrosion Resistance | Resistant in Saline Solutions | |
Valve Components | Friction & Wear Properties | Wear Resistance | |
Valve Components | Machining Properties | Machinability, Good | |
Valve Components | Mechanical Properties | Moderate Strength | |
Valves for Water Meters | Corrosion Resistance | Corrosion Resistance | |
Valves for Water Meters | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Valves for Water Meters | Corrosion Resistance | Resistant in Saline Solutions | |
Valves for Water Meters | Friction & Wear Properties | Wear Resistance | |
Valves for Water Meters | Machining Properties | Machinability, Good | |
Valves for Water Meters | Mechanical Properties | Moderate Strength | |
Marine | Marine Castings | Corrosion Resistance | Corrosion Resistance |
Marine Castings | Corrosion Resistance | Corrosion Resistance to Fresh Water | |
Marine Castings | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Marine Castings | Corrosion Resistance | Corrosion Resistance to Saline Solutions | |
Marine Castings | Machining Properties | Machinability, Good | |
Marine Castings | Mechanical Properties | Moderate Strength | |
Plumbing | Medium Pressure Steam Equipment to 550 F | Corrosion Resistance | Corrosion Resistance |
Medium Pressure Steam Equipment to 550 F | Corrosion Resistance | Corrosion Resistance to Numerous Environments | |
Medium Pressure Steam Equipment to 550 F | Machining Properties | Machinability, Good | |
Medium Pressure Steam Equipment to 550 F | Mechanical Properties | Moderate Strength | |
Medium Pressure Steam Equipment to 550 F | Mechanical Properties | Retains Strength at Elevated Temperatures | |
Medium Pressure Steam Equipment to 550 F | Pressure Tight | Pressure Tight to 260 C |
Form | Specific Sub-Form | Application | System | Standard | Description |
---|---|---|---|---|---|
As Centrifugal Cast | Castings | ASTM | B271/B271M | COPPER BASE ALLOY CENTRIFUGAL CASTINGS | |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
Castings | SAE | J462 | CAST COPPER ALLOYS | ||
As Continuous Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
Castings | ASTM | B505/B505M | COPPER BASE ALLOY CONTINUOUS CASTINGS | ||
As Sand Cast | Castings | SAE | J462 | CAST COPPER ALLOYS | |
Castings | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
Castings | ASTM | B584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
Castings | ASTM | B61 | STEAM OR VALVE BRONZE CASTINGS | ||
Castings | ASME | SB584 | COPPER ALLOY SAND CASTINGS FOR GENERAL APPLICATIONS | ||
Castings | ASME | SB61 | STEAM OR VALVE BRONZE CASTINGS | ||
Fitting | ASME | SB61 | STEAM OR VALVE BRONZE CASTINGS | ||
ASTM | B61 | STEAM OR VALVE BRONZE CASTINGS | |||
FEDERAL | WW-P-460 | PIPE FITTINGS: BRASS OR BRONZE | |||
ASME | B16.24 | BRONZE PIPE FLANGES AND FLANGED FITTINGS | |||
Flanges | ASTM | B61 | STEAM OR VALVE BRONZE CASTINGS | ||
ASME | SB61 | STEAM OR VALVE BRONZE CASTINGS | |||
FEDERAL | WW-P-460 | PIPE FITTINGS: BRASS OR BRONZE | |||
Ingot | |||||
ASTM | B30 | COPPER BASE ALLOYS IN INGOT FORM | |||
Valves | |||||
MILITARY | MIL-V-17547 | VALVE, CHECK, BRONZE |
Corrosion Properties
No Corrosion Properties Available.
DOWNLOAD Standard Designation for Wrought and Cast Alloys [PDF 775KB, includes all alloys]
PLEASE NOTE: This search is best used with Chrome, FFox 3.6+, Safari 2+, Opera 10+ and IE 9+. To report an issue with this page, please contact us.
DISCLAIMER:
The values listed above represent reasonable approximations suitable for general engineering use. Due to commercial variations in compositions and to manufacturing limitations, they should not be used for specification purposes. See applicable ASTM International specification references.
The values listed above represent reasonable approximations suitable for general engineering use. Due to commercial variations in compositions and to manufacturing limitations, they should not be used for specification purposes. See applicable ASTM International specification references.