C11000
Electrolytic Tough Pitch
ETP
Wrought
COPPERS
Coppers
true
true
https://api.copper.org/alloys.xhtml/C11000
Elements | |
---|---|
Cu(1,2,3) | |
(1) Oxygen and trace elements may vary depending on the process. (2) This is a high conductivity copper which has, in the annealed condition a minimum conductivity of 100% IACS. (3) Cu value includes Ag. |
|
Min (%) | 99.90 |
Max (%) |
Form | Temper | Temper Code | Tensile Strength (ksi) |
YS-0.5% Ext (ksi) |
Elongation (%) |
Rockwell B scale | Rockwell F scale | Rockwell 30T scale | Shear Strength (ksi) |
Torsion Modulus (ksi) |
Izod (ft-lbs) |
Fatigue Strength** (ksi) |
Ultimate Tensile Strength in Shear (ksi) |
Section Size (in) |
Cold Work (%) |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
* Measured at room temperature, 68°F (20°C). ** Fatigue Strength: 100 x 106 cycles, unless indicated as [N] x 106. | |||||||||||||||
Flat Products | 1/2 Hard | H02 |
42 Typ |
14 Typ |
40 Typ |
84 Typ |
50 Typ |
26 Typ |
13 Typ | 0.04 | |||||
1/4 Hard | H01 |
38 Typ |
30 Typ |
35 Typ |
25 Typ |
70 Typ |
25 Typ |
25 Typ |
0.025 | ||||||
1/4 Hard | H01 |
38 Typ |
30 Typ |
25 Typ |
25 Typ |
70 Typ |
36 Typ |
25 Typ |
0.04 | ||||||
1/8 Hard | H00 |
36 Typ |
28 Typ |
40 Typ |
10 Typ |
60 Typ |
25 Typ |
0.025 | |||||||
1/8 Hard | H00 |
36 Typ |
28 Typ |
30 Typ |
10 Typ |
60 Typ |
25 Typ |
25 Typ |
0.04 | ||||||
As Hot Rolled | M20 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.025 | ||||||||
As Hot Rolled | M20 |
34 Typ |
10 Typ |
45 Typ |
45 Typ |
23 Typ |
0.04 | ||||||||
Extra Spring | H10 |
57 Typ |
53 Typ |
4 Typ |
62 Typ |
95 Typ |
64 Typ |
29 Typ |
0.04 | ||||||
Hard | H04 |
50 Typ |
45 Typ |
12 Typ |
28 Typ |
0.24 | |||||||||
Hard | H04 |
50 Typ |
45 Typ |
6 Typ |
50 Typ |
90 Typ |
57 Typ |
28 Typ |
28 Typ |
0.04 | |||||
Hard | H04 |
45 Typ |
40 Typ |
20 Typ |
45 Typ |
85 Typ |
26 Typ |
1 | |||||||
Hard | H04 |
50 Typ |
45 Typ |
12 Typ |
50 Typ |
90 Typ |
28 Typ |
0.025 | |||||||
Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
45 Typ |
23 Typ |
11 Typ | 0.04 | |||||||
Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.025 | ||||||||
Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
0.04 | ||||||||
Spring | H08 |
55 Typ |
50 Typ |
4 Typ |
60 Typ |
94 Typ |
63 Typ |
29 Typ |
14 Typ | 0.04 | |||||
Rod | As Hot Rolled | M20 |
32 Typ |
55 Typ |
40 Typ |
22 Typ |
1 | ||||||||
Hard | H04 |
48 Typ |
44 Typ |
16 Typ |
47 Typ |
87 Typ |
27 Typ |
17 Typ | 1 | 35 | |||||
Hard | H04 |
45 Typ |
40 Typ |
20 Typ |
45 Typ |
85 Typ |
26 Typ |
6.4 Typ | 2 | 16 | |||||
Hard | H04 |
55 Typ |
50 Typ |
10 Typ |
60 Typ |
94 Typ |
29 Typ |
0.25 | 40 | ||||||
Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
55 Typ |
40 Typ |
22 Typ |
1 | ||||||||
Shapes | As Hot Extruded | M30 |
32 Typ |
50 Typ |
40 Typ |
22 Typ |
0.5 | ||||||||
As Hot Rolled | M20 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.5 | ||||||||
Hard | H04 |
40 Typ |
32 Typ |
30 Typ |
35 Typ |
26 Typ |
0.5 | 15 | |||||||
Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
50 Typ |
40 Typ |
22 Typ |
0.5 | ||||||||
Tube | Hard Drawn | H80 |
55 Typ |
8 Typ |
29 Typ |
40 | |||||||||
Hard Drawn | H80 |
55 Typ |
50 Typ |
8 Typ |
60 Typ |
95 Typ |
63 Typ |
29 Typ |
0.065 | 40 | |||||
Light Drawn, Light Cold Rolled | H55 |
40 Typ |
32 Typ |
25 Typ |
35 Typ |
77 Typ |
45 Typ |
26 Typ |
0.065 | 15 | |||||
Nominal Grain Size 0.025 mm | OS025 |
34 Typ |
11 Typ |
45 Typ |
45 Typ |
23 Typ |
0.065 | ||||||||
Nominal Grain Size 0.050 mm | OS050 |
32 Typ |
10 Typ |
45 Typ |
40 Typ |
22 Typ |
0.065 | ||||||||
Wire | Hard | H04 |
55 Typ |
1.5 Typ |
29 Typ |
0.08 | |||||||||
Nominal Grain Size 0.050 mm | OS050 |
35 Typ |
35 Typ |
24 Typ |
0.08 | ||||||||||
Spring | H08 |
66 Typ |
1.5 Typ |
33 Typ |
0.08 |
(1)Actual value .321 - .323.(2)Volume and weight basis. | |
Melting Point - Liquidus°F | 1981 |
---|---|
Melting Point - Solidus°F | 1949 |
Densitylb/cu in. at 68°F | 0.322 (1) |
Specific Gravity | 8.91 |
Electrical Conductivity% IACS at 68°F | 101 (2) |
Thermal ConductivityBtu/ sq ft/ ft hr/ °F at 68°F | 226 |
Coefficient of Thermal Expansion 68-21210 to -6 power per °F (68 – 212°F) | 9.4 |
Coefficient of Thermal Expansion 68-39210 to -6 power per °F (68 – 392°F) | 9.6 |
Coefficient of Thermal Expansion 68-57210 to -6 power per °F (68 – 572°F) | 9.8 |
Specific Heat CapacityBtu/ lb /°F at 68°F | 0.092 |
Modulus of Elasticity in Tensionksi | 17000 |
Modulus of Rigidityksi | 6400 |
Technique | Suitability |
---|---|
Soldering | Excellent |
Brazing | Good |
Oxyacetylene Welding | Not Recommended |
Gas Shielded Arc Welding | Fair |
Coated Metal Arc Welding | Not Recommended |
Spot Weld | Not Recommended |
Seam Weld | Not Recommended |
Butt Weld | Good |
Capacity for Being Cold Worked | Excellent |
Capacity for Being Hot Formed | Excellent |
Forgeability Rating | 65 |
Machinability Rating | 20 |
Common Fabrication Processes
- Blanking
- Coining
- Coppersmithing
- Drawing
- Etching
- Forming and Bending
- Heading and Upsetting
- Hot Forging and Pressing
- Piercing and Punching
- Roll Threading and Knurling
- Shearing
- Spinning
- Squeezing and Swaging
- Stamping
Treatment | Minimum* | Maximum* | ||
---|---|---|---|---|
* Temperature is measured in Fahrenheit. | ||||
Annealing | 700 | 1200 | ||
Hot Working Temperature | 1400 | 1600 |
Product Category | Product | Reason Category | Reason |
---|---|---|---|
Architecture | Building Fronts | Appearance | Appearance |
Building Fronts | Corrosion Resistance | Corrosion Resistance | |
Downspouts | Appearance | Appearance | |
Downspouts | Corrosion Resistance | Corrosion Resistance | |
Downspouts | Solderability | Solderability | |
Flashing | Appearance | Appearance | |
Flashing | Corrosion Resistance | Corrosion Resistance | |
Gutters | Appearance | Appearance | |
Gutters | Corrosion Resistance | Corrosion Resistance | |
Roofing | Appearance | Appearance | |
Roofing | Corrosion Resistance | Corrosion Resistance | |
Roofing | Solderability | Solderability | |
Skylight Frames | Appearance | Appearance | |
Skylight Frames | Corrosion Resistance | Corrosion Resistance | |
Spouting | Appearance | Appearance | |
Spouting | Corrosion Resistance | Corrosion Resistance | |
Spouting | Forming Characteristics | Formability | |
Automotive | Gaskets | Forming Characteristics | Formability |
Gaskets | Mechanical Properties | Ductiltiy | |
Gaskets | Pressure Tight | Pressure Tight | |
Radiators | Brazing Characteristics | Brazability | |
Radiators | Conductivity (Thermal) | Thermal Conductivity | |
Radiators | Corrosion Resistance | Corrosion Resistance | |
Radiators | Mechanical Properties | Creep Resistance | |
Radiators | Solderability | Solderability | |
Builders Hardware | Ball Floats | Corrosion Resistance | Corrosion Resistance |
Ball Floats | Forming Characteristics | Formability | |
Butts | Appearance | Appearance | |
Butts | Corrosion Resistance | Corrosion Resistance | |
Butts | Forming Characteristics | Formability | |
Cotter Pins | Corrosion Resistance | Corrosion Resistance | |
Cotter Pins | Mechanical Properties | Ductiltiy | |
Nails | Appearance | Appearance | |
Nails | Corrosion Resistance | Corrosion Resistance | |
Rivets | Appearance | Appearance | |
Rivets | Corrosion Resistance | Corrosion Resistance | |
Soldering Copper | Solderability | Solderability | |
Tacks | Appearance | Appearance | |
Tacks | Corrosion Resistance | Corrosion Resistance | |
Building | Screening | Appearance | Appearance |
Screening | Corrosion Resistance | Corrosion Resistance | |
Screening | Forming Characteristics | Formability | |
Wire Screening | Appearance | Appearance | |
Wire Screening | Corrosion Resistance | Corrosion Resistance | |
Wire Screening | Forming Characteristics | Formability | |
Consumer | Christmas Ornaments | Appearance | Appearance |
Christmas Ornaments | Forming Characteristics | Formability | |
Electrical | Busbars | Conductivity (Electrical) | Electrical Conductivity |
Busbars | Conductivity (Thermal) | Thermal Conductivity | |
Busbars | Corrosion Resistance | Corrosion Resistance | |
Conductors, Electrical | Conductivity (Electrical) | Electrical Conductivity | |
Conductors, Electrical | Conductivity (Thermal) | Thermal Conductivity | |
Conductors, Electrical | Corrosion Resistance | Corrosion Resistance | |
Contacts | Conductivity (Electrical) | Electrical Conductivity | |
Contacts | Conductivity (Thermal) | Thermal Conductivity | |
Contacts | Corrosion Resistance | Corrosion Resistance | |
Contacts | Solderability | Solderability | |
Magnet Wire | Conductivity (Electrical) | Electrical Conductivity | |
Magnet Wire | Conductivity (Thermal) | Thermal Conductivity | |
Magnet Wire | Corrosion Resistance | Corrosion Resistance | |
Magnet Wire | Non-Magnetic | Non-Magnetic | |
Radio Parts | Conductivity (Electrical) | Electrical Conductivity | |
Radio Parts | Conductivity (Thermal) | Thermal Conductivity | |
Radio Parts | Corrosion Resistance | Corrosion Resistance | |
Radio Parts | Solderability | Solderability | |
Stranded Conductors | Conductivity (Electrical) | Electrical Conductivity | |
Stranded Conductors | Conductivity (Thermal) | Thermal Conductivity | |
Stranded Conductors | Forming Characteristics | Formability | |
Switches | Conductivity (Electrical) | Electrical Conductivity | |
Switches | Conductivity (Thermal) | Thermal Conductivity | |
Switches | Corrosion Resistance | Corrosion Resistance | |
Switches | Solderability | Solderability | |
Terminal Connectors | Conductivity (Electrical) | Electrical Conductivity | |
Terminal Connectors | Conductivity (Thermal) | Thermal Conductivity | |
Terminal Connectors | Corrosion Resistance | Corrosion Resistance | |
Terminals | Conductivity (Electrical) | Electrical Conductivity | |
Terminals | Conductivity (Thermal) | Thermal Conductivity | |
Terminals | Corrosion Resistance | Corrosion Resistance | |
Terminals | Solderability | Solderability | |
Trolley Wire | Conductivity (Electrical) | Electrical Conductivity | |
Trolley Wire | Conductivity (Thermal) | Thermal Conductivity | |
Trolley Wire | Corrosion Resistance | Corrosion Resistance | |
Trolley Wire | Corrosion Resistance | Oxidation Resistance | |
Wire, Electrical | Conductivity (Electrical) | Electrical Conductivity | |
Wire, Electrical | Forming Characteristics | Formability | |
Fasteners | Fasteners | Appearance | Appearance |
Fasteners | Conductivity (Electrical) | Electrical Conductivity | |
Fasteners | Corrosion Resistance | Corrosion Resistance | |
Industrial | Anodes | Conductivity (Electrical) | Electrical Conductivity |
Chemical Process Equipment | Corrosion Resistance | Corrosion Resistance | |
Chemical Process Equipment | Forming Characteristics | Formability | |
Chemical Process Equipment | Solderability | Solderability | |
Chimney Cap Screens | Appearance | Appearance | |
Chimney Cap Screens | Corrosion Resistance | Corrosion Resistance | |
Chlorine Cells | Conductivity (Thermal) | Thermal Conductivity | |
Chlorine Cells | Corrosion Resistance | Corrosion Resistance | |
Heat Exchangers | Conductivity (Thermal) | Thermal Conductivity | |
Heat Exchangers | Corrosion Resistance | Corrosion Resistance | |
Kettles | Appearance | Appearance | |
Kettles | Conductivity (Thermal) | Thermal Conductivity | |
Kettles | Corrosion Resistance | Corrosion Resistance | |
Pans | Appearance | Appearance | |
Pans | Conductivity (Thermal) | Thermal Conductivity | |
Pans | Corrosion Resistance | Corrosion Resistance | |
Pressure Vessels | Conductivity (Thermal) | Thermal Conductivity | |
Pressure Vessels | Corrosion Resistance | Corrosion Resistance | |
Pressure Vessels | Forming Characteristics | Formability | |
Printing Rolls | Conductivity (Electrical) | Electrical Conductivity | |
Printing Rolls | Conductivity (Thermal) | Thermal Conductivity | |
Printing Rolls | Corrosion Resistance | Corrosion Resistance | |
Road Bed Expansion Plates | Conductivity (Thermal) | Thermal Conductivity | |
Road Bed Expansion Plates | Corrosion Resistance | Corrosion Resistance | |
Rotating Bands | Conductivity (Thermal) | Thermal Conductivity | |
Rotating Bands | Corrosion Resistance | Corrosion Resistance | |
Vats | Conductivity (Thermal) | Thermal Conductivity | |
Vats | Corrosion Resistance | Corrosion Resistance |
Form | Specific Sub-Form | Application | System | Standard | Description |
---|---|---|---|---|---|
ASTM | B224 | Standard Classification of Coppers | |||
Bands | Projectile Rotating | MILITARY | MIL-B-20292 | BLANKS, ROTATING BAND, FOR PROJECTILES | |
Bar | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | |||
SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
Bolts | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
Brazing Filler Metal | FEDERAL | QQ-B-650 | BRAZING ALLOY, COPPER, COPPER-ZINC, AND COPPER-PHOSPHORUS | ||
Bus Bar, Rod and Shapes, General Purpose, same | Bus Bar | ASTM | B187/B187M | COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES | |
ASME | SB187 | COPPER BUS BAR, ROD AND SHAPES AND GENERAL PURPOSE ROD, BAR AND SHAPES | |||
Die | Forgings | ASTM | B283/B283M | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | |
Foil | Printed Circuits | ASTM | B451 | COPPER FOIL, STRIP AND SHEET FOR PRINTED CIRCUITS AND CARRIER TAPES | |
Forgings, Die (Hot Pressed) | ASME | SB283 | COPPER AND COPPER ALLOY DIE FORGINGS (HOT PRESSED) | ||
Nuts | ASTM | F467 | NONFERROUS NUTS FOR GENERAL USE | ||
Pipe | Bus Bar | ASTM | B188 | SEAMLESS COPPER BUS PIPE AND TUBE | |
Plate | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
AMS | 4500 | COPPER SHEET, STRIP AND PLATE, SOFT ANNEALED | |||
SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
Rod | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
MILITARY | MIL-C-12166 | COPPER ROD FOR CRUSHER CYLINDERS OR PRESSURE CYLINDERS | |||
SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
Forgings | ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | ||
Screws | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
Shapes | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | ||
SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
ASTM | B124/B124M | COPPER AND COPPER-ALLOY FORGING ROD, BAR AND SHAPES | |||
Sheet | ASTM | B694 | COPPER, COPPER ALLOY AND COPPER-CLAD STAINLESS STEEL SHEET AND STRIP FOR ELECTRICAL CABLE SHIELDING | ||
Building Construction | ASTM | B370 | COPPER SHEET AND STRIP FOR BUILDING CONSTRUCTION | ||
AMS | 4500 | COPPER SHEET, STRIP AND PLATE, SOFT ANNEALED | |||
SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
ASTM | B506 | COPPER CLAD STAINLESS STEEL SHEET AND STRIP FOR BUILDING CONSTRUCTION | |||
Printed Circuits | ASTM | B451 | COPPER FOIL, STRIP AND SHEET FOR PRINTED CIRCUITS AND CARRIER TAPES | ||
SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | |||
Sheet, Strip, Roller Bar & Plate | ASME | SB152 | COPPER SHEET, STRIP, PLATE, AND ROLLED BAR | ||
ASTM | B152/B152M | COPPER SHEET, STRIP, PLATE AND ROLLED BAR | |||
Strip | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
Building Construction | ASTM | B370 | COPPER SHEET AND STRIP FOR BUILDING CONSTRUCTION | ||
ASTM | B272 | COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP) | |||
AMS | 4500 | COPPER SHEET, STRIP AND PLATE, SOFT ANNEALED | |||
ASTM | B506 | COPPER CLAD STAINLESS STEEL SHEET AND STRIP FOR BUILDING CONSTRUCTION | |||
ASTM | B694 | COPPER, COPPER ALLOY AND COPPER-CLAD STAINLESS STEEL SHEET AND STRIP FOR ELECTRICAL CABLE SHIELDING | |||
SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |||
Printed Circuits | ASTM | B451 | COPPER FOIL, STRIP AND SHEET FOR PRINTED CIRCUITS AND CARRIER TAPES | ||
Studs | ASTM | F468 | NONFERROUS BOLTS, HEX CAP SCREWS, AND STUDS FOR GENERAL USE | ||
Tube | Bus Bar | ASTM | B188 | SEAMLESS COPPER BUS PIPE AND TUBE | |
ASTM | B447 | WELDED COPPER TUBE | |||
Wire | Soft | SAE | J463 | WROUGHT COPPER AND COPPER ALLOYS | |
Hard Drawn | ASTM | B2 | MEDIUM-HARD DRAWN COPPER WIRE | ||
ASTM | B189 | LEAD-COATED AND LEAD ALLOY COATED SOFT COPPER WIRE FOR ELECTRICAL PURPOSES | |||
Soft | FEDERAL | QQ-W-343 | WIRE, ELECTRICAL (UNINSULATED) | ||
FEDERAL | QQ-B-575 | BRAID, WIRE (COPPER, TIN-COATED OR SILVER-COATED, TUBULAR OR FLAT) | |||
Hard Drawn | FEDERAL | QQ-W-343 | WIRE, ELECTRICAL (UNINSULATED) | ||
ASTM | B246 | TINNED HARD-DRAWN AND MEDIUM HARD-DRAWN COPPER WIRE FOR ELECTRICAL PURPOSES | |||
ASTM | B355 | NICKEL-COATED SOFT OR ANNEALED COPPER WIRE | |||
ASTM | B272 | COPPER FLAT PRODUCTS WITH FINISHED (ROLLED OR DRAWN) EDGES (FLAT WIRE AND STRIP) | |||
ASTM | B226 | CORED, ANNULAR, CONCENTRIC-LAY-STRANDED COPPER CONDUCTORS | |||
Hard Drawn | ASTM | B1 | HARD-DRAWN COPPER WIRE | ||
Trolly | ASTM | B116 | FIGURE 9 DEEP-SECTION GROOVED AND FIGURE 8 COPPER TROLLEY WIRE FOR INDUSTRIAL HAULAGE | ||
ASTM | B470 | BONDED COPPER CONDUCTORS FOR USE IN HOOKUP WIRE FOR ELECTRONIC EQUIPMENT | |||
Soft | ASTM | B738 | FINE-WIRE BUNCH-STRANDED AND ROPE-LAY BUNCH STRANDED COPPER CONDUCTORS FOR USE AS ELECTRICAL CONDUCT | ||
Hard Drawn | FEDERAL | QQ-W-343 | WIRE, ELECTRICAL (UNINSULATED) | ||
ASTM | B286 | COPPER CONDUCTORS FOR HOOKUP WIRE IN ELECTRONIC EQUIPMENT | |||
ASTM | B496 | COMPACT ROUND CONCENTRIC-LAY-STRANDED COPPER CONDUCTORS | |||
ASTM | B173 | ROPE-LAY-STRANDED CONDUCTORS WITH CONCENTRIC STRANDED MEMBERS | |||
ASTM | B174 | BUNCH-STRANDED CONDUCTORS | |||
ASTM | B172 | ROPE-LAY-STANDARD CONDUCTORS WITH BUNCH STRANDED MEMBERS | |||
ASTM | B33 | TINNED SOFT OR ANNEALED COPPER WIRE FOR ELECTRICAL PURPOSES | |||
ASTM | B298 | SILVER-COATED SOFT OR ANNEALED COPPER WIRE | |||
ASTM | B8 | CONCENTRIC-LAY-STRANDED COPPER CONDUCTORS, HARD, MEDIUM-HARD OR SOFT | |||
Soft | ASTM | B48 | SOFT RECTANGULAR AND SQUARE BARE COPPER WIRE FOR ELECTRICAL CONDUCTORS | ||
ASTM | B229 | CONCENTRIC-LAY-STRANDED COPPER AND COPPER-CLAD STEEL COMPOSITE CONDUCTORS | |||
Soft | ASTM | B3 | SOFT OR ANNEALED COPPER WIRE | ||
Soft | SAE | J461 | WROUGHT AND CAST COPPER ALLOYS | ||
Trolly | ASTM | B47 | COPPER TROLLEY WIRE | ||
MILITARY | MIL-W-6712 | WIRE, METALLIZING |
Corrosion Properties
No Corrosion Properties Available.
DOWNLOAD Standard Designation for Wrought and Cast Alloys [PDF 775KB, includes all alloys]
PLEASE NOTE: This search is best used with Chrome, FFox 3.6+, Safari 2+, Opera 10+ and IE 9+. To report an issue with this page, please contact us.
DISCLAIMER:
The values listed above represent reasonable approximations suitable for general engineering use. Due to commercial variations in compositions and to manufacturing limitations, they should not be used for specification purposes. See applicable ASTM International specification references.
The values listed above represent reasonable approximations suitable for general engineering use. Due to commercial variations in compositions and to manufacturing limitations, they should not be used for specification purposes. See applicable ASTM International specification references.