Resources
- Find Suppliers of Copper
- Technical Reference Library
- Publications List
- Automotive
- Building Construction: Air Conditioning / Heating
- Building Construction: Architecture
- Building Construction: Fire Sprinklers
- Building Construction: Home Builders' Marketing Materials
- Building Construction: Natural Gas
- Building Construction: Plumbing
- Electrical: Energy Efficiency
- Electrical: General
- Electrical: Power Quality
- Electrical: Telecommunications
- Industrial: Bronze Bearings
- Industrial: Cast Products
- Industrial: General
- Industrial: Machined Rod Products
- Industrial: Mold Alloys
- Properties / Standards
- Seawater
- Soldering / Brazing / Welding
- Special Publications
- Statistics / Directories
- Automotive
- Market Data
- Standards + Properties
- Properties of Wrought and Cast Copper Alloys
- Typical Uses of Copper Alloys
- Microstructures of Copper Alloys
- Corrosion Protection & Resistance
- Fabrication Practices
- Properties of Copper
- ASTM Standard Designation for Wrought and Cast Copper and Copper Alloys
- Powder Metallurgy
- Advantages and Applications of Copper
- Appendix A
- Appendix B
- Appendix C
- Applications of Copper-Base Powder Metals
- Characteristics and Properties
- Copper Powder Consolidation Techniques
- Copper in Iron and Steel P/M Parts
- Engineering / Production / Economic Advantages
- Nonstructural Applications of Copper
- Production and Properties
- Advantages and Applications of Copper
- Metallurgy of Copper-Base Alloys
- Mechanical Properties of Copper at Low Temperatures
- Standard Designation for Wrought and Cast Copper
- International Alloy Systems for Copper
- Comparison of National Standards
- Cross Specification Index
- European Numbering System for Non-Ferrous Metals
- Properties of Wrought and Cast Copper Alloys
Coppers
Overview
The major uses of pure, unalloyed copper are based on its high electrical and thermal conductivity as well its good corrosion resistance. Almost all alloying elements are detrimental to the electrical conductivity of copper, making the purity of the mental an important issue. Commercially pure copper is represented by UNS numbers C10100 to C13000. The various grades of unalloyed copper differ in the amount of impurities and therefore do behave differently. Oxygen free coppers are used in applications requiring high conductivity and exceptional ductility.
The pure copper or high copper alloys are made from copper ores that are obtained from the mines as sulfides, which contain zinc, lead and other sulfur. The ores are crushed and milled until they becomes a powder. A technique known as flotation separates the metal from the non-metal components of the powder. The next step is a concentrating stage where minerals are concentrated into a slurry that is about 15% copper. The copper is then melted and purified in several stages until it is 99% pure copper. At this point it is cast into anodes. Oxygen remains in the structure as cuprous oxide, Cu2O. The majority of the structure is pure copper. The copper metal solidifies from the liquid state by the growth of crystals. The crystals grow in preferred directions and form open, tree like structures called dendrites. The dendritic structure is very typical of cast metals. A lower melting point mixture of pure copper and cupprous oxide, called a eutectic, forms in the open spaces between the dendrites. The eutectic particles are usually dark, globular bodies dispersed in a copper background. The cuprous oxide particles form a network, outlining the dendritic cells. Pores, seen as dark spots in the microstructure, are also present in the as-cast material.
The copper anodes are then refined electrolytically to 99.9% purity. Copper melted under non oxidizing conditions is called oxygen free copper. The most popular form of pure copper is the standard electrical wire grade of copper (C11000) contains 99.95% Cu, 0.03% O2, and less than 50 ppm metallic impurities. It has a high electrical conductivity, in excess of 100% IACS. In the as cast form it is called electrolytic tough pitch (ETP) copper. The structure of the as-cast material is similar to that described above. When the as-cast ETP copper is hot rolled the eutectic structure is completely destroyed. The microstructure of the hot rolled copper contains many small grains. Parallel straight lines extending across many of the grains are called annealing twins. They appear after a metal has been mechanically worked at a high temperature, called annealing, and deformed. The interdendritic network of cupprous oxide particles was destroyed by hot rolling. After hot rolling, cupprous oxide particles changed form, and are present as stringers or aligned rows of dark particles. The oxide particles are much larger and fewer in number than in the as cast microstructure.
NOTE: The file size of the Larger and Largest View of the Micrographs are substantially larger than the thumbnail shown. The Larger View images range in size from 11K to 120K depending on the image. The Largest View images range in size from 125K to almost 500K.
| Alloy Family: | Coppers | |
|---|---|---|
| Product Form: | ||
| Processing: | Hot extruded | |
| Etchant: | Urquhart's Reagent | |
| Scale Line Length: | ~ 250Microns | |
| Alloy: | ||
| Temper: | ||
| Material: | Copper | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Wire | |
| Processing: | Continuous cast 5/16" dia rod, annealed 30 min at 700C drawn to .081" dia, annealed 2 hr at 200C, | |
| Etchant: | ||
| Scale Line Length: | ~ 25Microns | |
| Alloy: | ||
| Temper: | ||
| Material: | Copper | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Wire | |
| Processing: | Continuous cast, 5/16" dia, hot rolled rod, drawn to .081 dia, hard wire, not annealed | |
| Etchant: | ||
| Scale Line Length: | ~ 25Microns | |
| Alloy: | ||
| Temper: | ||
| Material: | Copper | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Wire | |
| Processing: | Continuous cast hot rolled 5/16" diameter, hot rolled rod drawn to .081 d hard wire, not annealed | |
| Etchant: | ||
| Scale Line Length: | ~ 25Microns | |
| Alloy: | ||
| Temper: | ||
| Material: | Copper | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Wire | |
| Processing: | Continuous cast hot rolled rod, annealed 30 min at 700 C, drawn to .081 dia, annealed 2 hr at 200 c | |
| Etchant: | ||
| Scale Line Length: | ~ 25Microns | |
| Alloy: | ||
| Temper: | ||
| Material: | Copper | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Rod | |
| Processing: | ||
| Etchant: | ||
| Scale Line Length: | ~ 125Microns | |
| Alloy: | C10100 | |
| Temper: | ||
| Material: | Copper OFHC | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Cast | |
| Processing: | As cast | |
| Etchant: | ||
| Scale Line Length: | ~ 50Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Cast | |
| Processing: | As cast | |
| Etchant: | ||
| Scale Line Length: | ~ 125Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | ||
| Processing: | Embrittled | |
| Etchant: | ||
| Scale Line Length: | ~ 125Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Wire | |
| Processing: | Hot rolled | |
| Etchant: | ||
| Scale Line Length: | ~ 50Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Wire | |
| Processing: | Soft annealed | |
| Etchant: | ||
| Scale Line Length: | ~ 50Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
Description: |
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Rod | |
| Processing: | Continuous cast, 5/16" dia, hot rolled rod | |
| Etchant: | ||
| Scale Line Length: | ~ 250Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
Description: |
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Rod | |
| Processing: | Continuous cast, 5/16" dia, hot rolled rod | |
| Etchant: | ||
| Scale Line Length: | ~ 250Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
Description: |
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Rod | |
| Processing: | Continuous cast, 5/16" dia. hot rolled rod | |
| Etchant: | ||
| Scale Line Length: | ~ 50Microns | |
| Alloy: | C11000 | |
| Temper: | ||
| Material: | ETP | |
| Source: | University of Florida |
|
Alloy Family: | Coppers |
|---|---|---|
| Product Form: | Cast | |
| Processing: | As cast | |
| Etchant: | ||
| Scale Line Length: | ~ 500Microns | |
| Alloy: | C12200 | |
| Temper: | ||
| Material: | DHP | |
| Source: | University of Florida |