Table 14.2a. Dimensions and Physical Characteristics of Copper Tube: Type K

Nominal or standard size, inchesNominal dimensions, inchesCalculated values (based on nominal dimensions)
Outside diameterInside diameterWall thicknessCross sectional area of bore, sq. inchesWeight of tube only, pounds per linear ft.Weight of tube & water, pounds per linear ft.Volume of tube, per linear ft.
Cu ft.Gal.
14 .375 .305 .035 .073 .145 .177 .00051 .00379
38 .500 .402 .049 .127 .269 .324 .00088 .00660
12 .625 .527 .049 .218 .344 .438 .00151 .0113
58 .750 .652 .049 .334 .418 .562 .00232 .0174
34 .875 .745 .065 .436 .641 .829 .00303 .0227
1 1.125 .995 .065 .778 .839 1.18 .00540 .0404
114 1.375 1.245 .065 1.22 1.04 1.57 .00847 .0634
112 1.625 1.481 .072 1.72 1.36 2.10 .0119 .0894
2 2.125 1.959 .083 3.01 2.06 3.36 .0209 .156
212 2.625 2.435 .095 4.66 2.93 4.94 .0324 .242
3 3.125 2.907 .109 6.64 4.00 6.87 .0461 .345
312 3.625 3.385 .120 9.00 5.12 9.01 .0625 .468
4 4.125 3.857 .134 11.7 6.51 11.6 .0813 .608
5 5.125 4.805 .160 18.1 9.67 17.5 .126 .940
6 6.125 5.741 .192 25.9 13.9 25.1 .180 1.35
8 8.125 7.583 .271 45.2 25.9 45.4 .314 2.35
10 10.125 9.449 .338 70.1 40.3 70.6 .487 3.64
12 12.125 11.315 .405 101 57.8 101 .701 5.25