| Dimensions, In. | Area | Weight Per Foot, Lb | DC Resistance at 20° C, Microhms Per Ft | |
|---|---|---|---|---|
| Square In. | Circular Mils, Thousands | |||
| 1/16 x 1/2 1/16 x 3/4 1/16 x 1 1/16 x 1 1/2 1/16 x 2 |
0.0312 0.0469 0.0625 0.0938 0.125 |
39.7 59.7 79.6 119 159 |
0.121 0.181 0.241 0.362 0.483 |
264.0 175.0 132.0 87.7 65.8 |
| 1/8 x 1/2 1/8 x 3/4 1/8 x 1 1/8 x 1 1/2 1/8 x 2 1/8 x 2 1/2 1/8 x 3 1/8 x 3 1/2 1/8 x 4 |
0.0625 0.0938 0.125 0.188 0.250 0.312 0.375 0.438 0.500 |
79.6 119 159 239 318 397 477 558 636 |
0.241 0.362 0.483 0.726 0.966 1.21 1.45 1.69 1.93 |
132.0 87.7 65.8 43.8 32.9 26.4 21.9 18.8 16.5 |
| 3/16 x 1/2 3/16 x 3/4 3/16 x 1 3/16 x 1 1/2 3/16 x 2 3/16 x 2 1/2 3/16 x 3 3/16 x 3 1/2 3/16 x 4 |
0.0938 0.141 0.188 0.281 0.375 0.469 0.562 0.656 0.750 |
119 179 239 358 477 597 715 835 955 |
0.362 0.545 0.726 1.09 1.45 1.81 2.17 2.53 2.90 |
87.7 58.4 43.8 29.3 21.9 17.5 14.6 12.5 11.0 |
| 1/4 x 1/2 1/4 x 3/4 1/4 x 1 1/4 x 1 1/2 1/4 x 2 1/4 x 2 1/2 1/4 x 3 1/4 x 3 1/2 1/4 x 4 1/4 x 5 1/4 x 6 1/4 x 8 1/4 x 10 1/4 x 12 |
0.125 0.188 0.250 0.375 0.500 0.625 0.750 0.875 1.00 1.25 1.50 2.00 2.50 3.00 |
159 239 318 477 637 796 955 1,110 1,270 1,590 1,910 2,550 3,180 3,820 |
0.483 0.726 0.966 1.45 1.93 2.41 2.90 3.38 3.86 4.83 5.80 7.73 9.66 11.6 |
65.8 43.8 32.9 21.9 16.5 13.2 11.0 9.40 8.23 6.58 5.49 4.11 3.29 2.74 |
| 3/8 x 3/4 3/8 x 1 3/8 x 1 1/2 3/8 x 2 3/8 x 2 1/2 3/8 x 3 3/8 x 3 1/2 3/8 x 4 3/8 x 5 3/8 x 6 3/8 x 8 3/8 x 10 3/8 x 12 |
0.281 0.375 0.562 0.750 0.938 1.12 1.31 1.50 1.88 2.25 3.00 3.75 4.50 |
358 477 715 955 1,190 1,430 1,670 1,910 2,390 2,860 3,820 4,770 5,730 |
1.09 1.45 2.17 2.90 3.62 4.35 5.06 5.80 7.26 8.69 11.6 14.5 17.4 |
29.3 21.9 14.6 11.0 8.77 7.35 6.28 5.49 4.38 3.66 2.74 2.19 1.83 |
| 1/2 x 1 1/2 x 1 1/2 1/2 x 2 1/2 x 2 1/2 1/2 x 3 1/2 x 3 1/2 1/2 x 4 1/2 x 5 1/2 x 6 1/2 x 8 1/2 x 10 1/2 x 12 |
0.500 0.750 1.00 1.25 1.50 1.75 2.00 2.50 3.00 4.00 5.00 6.00 |
637 955 1,270 1,590 1,910 2,230 2,550 3,180 3,820 5,090 6,360 7,640 |
1.93 2.90 3.86 4.83 5.80 6.76 7.73 9.66 11.6 15.5 19.3 23.2 |
16.5 11.0 8.23 6.58 5.49 4.70 4.11 3.29 2.74 2.06 1.65 1.37 |
| 3/4 x 4 3/4 x 5 3/4 x 6 3/4 x 8 3/4 x 10 3/4 x 12 |
3.00 3.75 4.50 6.00 7.50 9.00 |
3,820 4,770 5,730 7,640 9,550 11,500 |
11.6 14.5 17.4 23.2 29.0 34.8 |
2.74 2.19 1.83 1.37 1.10 0.914 |
| Dimensions, In. | 30 °C Rise | 50 °C Rise | 65 °C Rise | |||
|---|---|---|---|---|---|---|
| Skin Effect Ratio at 70° C | 60-Hz Ampacity,* Amp | Skin Effect Ratio at 90° C | 60-Hz Ampacity, *Amp | Skin Effect Ratio at 105° C | 60-Hz Ampacity, *Amp | |
| 1/16 x 1/2 1/16 x 3/4 1/16 x 1 1/16 x 1 1/2 1/16 x 2 |
1.00 1.00 1.00 1.00 1.01 |
103 145 187 270 345 |
1.00 1.00 1.00 1.00 1.01 |
136 193 250 355 460 |
1.00 1.00 1.00 1.00 1.01 |
157 225 285 410 530 |
| 1/8 x 1/2 1/8 x 3/4 1/8 x 1 1/8 x 1 1/2 1/8 x 2 1/8 x 2 1/2 1/8 x 3 1/8 x 3 1/2 1/8 x 4 |
1.00 1.00 1.01 1.01 1.02 1.02 1.03 1.04 1.04 |
153 215 270 385 495 600 710 810 910 |
1.00 1.00 1.01 1.01 1.02 1.02 1.03 1.03 1.04 |
205 285 360 510 660 800 940 1,100 1,200 |
1.00 1.00 1.01 1.01 1.02 1.02 1.03 1.03 1.04 |
235 325 415 590 760 920 1,100 1,250 1,400 |
| 3/16 x 1/2 3/16 x 3/4 3/16 x 1 3/16 x 1 1/2 3/16 x 2 3/16 x 2 1/2 3/16 x 3 3/16 x 3 1/2 3/16 x 4 |
1.00 1.01 1.01 1.02 1.03 1.04 1.05 1.07 1.09 |
195 270 340 480 610 740 870 990 1,100 |
1.00 1.01 1.01 1.02 1.03 1.04 1.05 1.06 1.08 |
260 360 455 630 810 980 1,150 1,300 1,450 |
1.00 1.01 1.01 1.02 1.03 1.03 1.04 1.06 1.07 |
300 415 520 730 940 1,150 1,350 1,500 1,700 |
| 1/4 x 1/2 1/4 x 3/4 1/4 x 1 1/4 x 1 1/2 1/4 x 2 1/4 x 2 1/2 1/4 x 3 1/4 x 3 1/2 1/4 x 4 1/4 x 5 1/4 x 6 1/4 x 8 1/4 x 10 1/4 x 12 |
1.01 1.01 1.02 1.03 1.04 1.06 1.08 1.10 1.12 1.16 1.18 1.23 1.27 1.31 |
240 320 400 560 710 850 990 1,150 1,250 1,500 1,750 2,250 2,700 3,150 |
1.01 1.01 1.02 1.03 1.04 1.06 1.08 1.09 1.11 1.15 1.17 1.22 1.26 1.30 |
315 425 530 740 940 1,150 1,300 1,500 1,700 2,000 2,350 3,000 3,600 4,200 |
1.01 1.01 1.02 1.03 1.04 1.06 1.07 1.09 1.10 1.14 1.17 1.21 1.25 1.28 |
360 490 620 860 1,100 1,300 1,550 1,750 1,950 2,350 2,700 3,450 4,200 4,900 |
| 3/8 x 3/4 3/8 x 1 3/8 x 1 1/2 3/8 x 2 3/8 x 2 1/2 3/8 x 3 3/8 x 3 1/2 3/8 x 4 3/8 x 5 3/8 x 6 3/8 x 8 3/8 x 10 3/8 x 12 |
1.02 1.03 1.05 1.08 1.12 1.15 1.18 1.20 1.24 1.27 1.33 1.38 1.42 |
415 510 710 880 1,050 1,200 1,350 1,500 1,800 2,100 2,650 3,200 3,700 |
1.02 1.03 1.04 1.08 1.10 1.14 1.16 1.19 1.23 1.26 1.31 1.36 1.40 |
550 680 940 1,150 1,400 1,600 1,800 2,000 2,400 2,800 3,550 4,300 5,000 |
1.02 1.03 1.04 1.07 1.09 1.13 1.15 1.18 1.22 1.24 1.30 1.35 1.38 |
630 790 1,100 1,350 1,600 1,850 2,100 2,350 2,800 3,250 4,100 4,900 5,800 |
| 1/2 x 1 1/2 x 1 1/2 1/2 x 2 1/2 x 2 1/2 1/2 x 3 1/2 x 3 1/2 1/2 x 4 1/2 x 5 1/2 x 6 1/2 x 8 1/2 x 10 1/2 x 12 |
1.04 1.08 1.12 1.16 1.20 1.24 1.26 1.32 1.36 1.42 1.47 1.52 |
620 830 1,000 1,200 1,400 1,550 1,700 2,050 2,400 3,000 3,600 4,200 |
1.04 1.08 1.11 1.15 1.19 1.22 1.25 1.30 1.34 1.40 1.45 1.51 |
820 1,100 1,350 1,600 1,850 2,100 2,300 2,750 3,150 4,000 4,800 5,600 |
1.04 1.07 1.10 1.14 1.18 1.21 1.24 1.29 1.33 1.39 1.44 1.50 |
940 1,250 1,550 1,850 2,150 2,400 2,650 3,150 3,650 4,600 5,500 6,400 |
| 3/4 x 4 3/4 x 5 3/4 x 6 3/4 x 8 3/4 x 10 3/4 x 12 |
1.42 1.48 1.52 1.60 1.67 1.72 |
2,050 2,400 2,800 3,500 4,200 4,900 |
1.40 1.46 1.50 1.58 1.64 1.69 |
2,750 3,250 3,750 4,700 5,600 6,500 |
1.38 1.44 1.48 1.56 1.62 1.67 |
3,150 3,750 4,300 5,400 6,500 7,500 |
| * Applicable to typical in-service conditions (indoors, 40°C ambient temperature), horizontal run on edge, and free from external magnetic influences. | ||||||